Table 160.055-3(j)
Property | Test method | Requirement |
Tensile strength | ASTM-D882, Method B, 1/2 in. dumbbell die | 1,200 p.s.i., minimum. |
Ultimate elongation | ASTM-D882, Method B, 1/2 in. dumbbell die | 320 percent, minimum. |
Tear resistance | ASTM-D1004, Constant Elongation Machine | 90 pounds per inch, minimum. |
Abrasion resistance | FS CCC-T-191, Method 5304, No. 8 cotton duck, 6 lb. tension, 2 lb. pressure | 100,000 double rubs. |
Blocking | FS CCC-T-191, Method 5872, 30 minutes at 180 °F., 1/4 p.s.i | No blocking. |
Accelerated weathering | FS CCC-T-191, Method 5670, 120 hours | Color change-very slight. Cracking-None. Flexibility-No change. |
Plasticizer heat loss | FS CCC-A-700, paragraph 4.4.4, 48 hours at 221 °F | 8 percent, maximum. |
Adhesion to foam-Tensile pull | ASTM-D413, machine method, 12 in. per minute, 1 in. strip | |
Film to foam skin | 4 lb./in., minimum. | |
Film to foam (no skin) | 2 lb./in., minimum. | |
Water absorption | ASTM-D570, 24 hours at 70 °F | 0.5 percent, maximum. |
Cold crack (unsupported film) 0 °F | Coast Guard, 164.015, paragraph 164.015-4(j) | No cracking. |
46 C.F.R. §160.055-3